By Mathias Alvarez, Roofing Masters Limited
The information in this article is based on our experience as membrane roofing applicators and is intended as a general guide only. Product specifications, performance and suitability can vary depending on the manufacturer, application conditions and specific project requirements.
When a butyl roof is tired but not finished, two coatings come up again and again for restoring it: water-based aliphatic polyurethane and high-solids moisture-cure silicone. Both work. They handle New Zealand’s sun, heat and salt air differently, though, and the one you choose now affects what you can do with that roof down the track from now.
Scope and basis
This article covers one situation. The existing butyl sheet is still serviceable but is nearing the end of its weathering life, and full replacement isn’t justified yet.
We’ve kept both systems generic. Coverage rates, film thicknesses and cure times are the ranges published across current manufacturers’ technical datasheets. On any real job, the datasheet for the specific product you’re using is the figure that counts, not this article.
What we don’t cover:
- Acrylic and asphaltic coatings. Neither is suitable over butyl in these conditions.
- Full membrane replacement.
- Torch-on and self-adhesive sheet overlays.
- Any roof where the substrate has failed structurally.
The relevant parts of the Building Code are Clause B2 Durability and Clause E2 External Moisture. Keep in mind that a coating extends the weathering life of the roof. It does not reset the durability clock on the butyl underneath.
The substrate: butyl after years in service
Butyl rubber (IIR, a copolymer of isobutylene and isoprene) has been used on New Zealand roofs for more than fifty years. It’s a single-ply synthetic rubber, supplied in black and grey, typically 1.0 to 1.5 mm thick. Laps are joined with solvent adhesive and seam tape. Appraised systems carry B2.3.1(b) fifteen-year durability and a stated serviceable life of at least twenty years.
In our experience in Nelson, grey butyl lasts better than black. Thin 1.0 mm black suffers a beating here, 1.5 mm black is a bit better, and 1.5 mm grey holds up much better. That’s what we’ve seen on roofs here in Nelson, not test data. It’s likely because black sheet runs hotter in the sun (see Heat below) on top of our high UV. It matters for restoration: thin black sheet is likely to be further through its life when you come to assess it, so check it sooner before it gets beyond coating.
In our experience the main sheet is rarely the first thing to fail. The usual order is:
- Lap adhesive creeps and the seams start to open.
- Movement shows up at flashings and penetrations.
- The surface hardens and develops a bloom from long-term oxidation.
- Physical damage builds up along foot traffic routes and around rooftop plant.
If the deck and any insulation are dry and the main sheet is sound, a coating deals with the problems that actually occur.
Getting the coating to stick
Adhesion makes or breaks the job. Butyl is an oily, low-energy rubber that resists bonding, for three reasons:
- Its surface doesn’t wet out easily, so water-based coatings tend to bead up rather than spread and grip.
- Processing oils and plasticisers keep working their way to the surface for the life of the sheet.
- Years of oxidation leave a chalky, crumbly layer on top that has no strength of its own.
No coating bonds to butyl just because it has been rolled on. The bond has to be built. There are two ways to do that: use a solvent to soften and reopen the rubber surface, or chemically treat the surface and bridge to it with a primer.
Before you specify anything
- A moisture survey, either an infrared survey to ASTM C1153 or a capacitance survey, with invasive moisture readings of the substrate and then patched.
- A field adhesion test on the actual membrane, after the planned preparation, cured for the manufacturer’s full stated period.
- Written confirmation that falls are positive and every outlet, sump and overflow is clear.
- A main sheet that is at least 80% sound, with wet substrate under less than about a quarter of the area.
CAUTION: A coating applied over trapped moisture seals the water in. In New Zealand’s humid coastal conditions that rots the deck from underneath, and you won’t see it until the failure is structural. The moisture survey is the cheapest line on the job and the one step that can never be skipped.
The New Zealand exposure environment
New Zealand has some of the highest UV levels of comparable developed countries in the temperate zone. In the upper South Island, the peak summer UV index reaches 12 to 13. That’s roughly 30 to 40% above the summer peak at the same latitude in the Northern Hemisphere. Three things add up:
- In early January, during our summer, the Earth is about 7% closer to the sun.
- The ozone layer over New Zealand is thinner than the northern mid-latitude average.
- Our clean maritime air has far less haze and dust to filter UV than the air over the northern continents.

Why silicone handles the sun
Every coating is held together by chemical bonds, and sunlight carries energy. If the energy in the UV is higher than the strength of a bond, it can break that bond and the coating slowly breaks down.
Most organic coatings are built on bonds that ground-level UV is strong enough to break. Silicone is built on a silicon–oxygen bond that is stronger than the energy in any sunlight reaching a New Zealand roof. Its UV resistance comes from that bond itself. It doesn’t depend on a stabiliser package.
For the technically minded: a UV photon at 295 nm carries about 406 kJ/mol and one at 400 nm about 299 kJ/mol. That range covers C–N (305), C–C (346) and C–O (358 kJ/mol) bonds. The silicon–oxygen (siloxane) bond sits near 452 kJ/mol, above anything that reaches the ground here.
How polyurethane copes
Aliphatic polyurethane is protected in a different way. UV can break its backbone bonds, but an aliphatic chain doesn’t absorb UV efficiently, so comparatively little of the sunlight gets absorbed and does damage. Chemists describe this as kinetic rather than thermodynamic protection.
Aromatic polyurethane is another matter. Left exposed to New Zealand sun, it yellows, chalks and goes brittle within months. Aromatic products belong under a topcoat and should never be the exposed surface.
Heat
On black butyl sheet, the surface can reach 70 to 80 °C in strong summer sun. On a clear winter night the same surface can drop below zero. A high-reflectance white finish cuts the peak surface temperature by 30 to 40 °C. A mid-grey finish gives you comparatively little of that benefit.
Solar Reflectance Index (SRI) combines how much sun a surface reflects with how well it sheds heat, giving one number for how hot it runs (higher means cooler). It mostly comes down to colour and the specific product rather than PU versus silicone, so compare like with like and use aged values where the manufacturer publishes them (for example, Cool Roof Rating Council aged ratings), as dirt pickup lowers SRI over time. It isn’t an NZ Building Code requirement.
The application window
Both systems need a substrate at or above roughly 5 °C and rising, with no rain, dew, fog or condensation during the cure period. In practice, October to April is the reliable window. May and September are marginal, and June to August is effectively shut.

System A: Water-based aliphatic polyurethane
This is a single-component, water-based product (an aqueous dispersion of aliphatic polyurethane). As the water evaporates, the polyurethane particles pack together and fuse into a continuous, elastic membrane. It’s solvent-free and low in VOCs, and the cured film stays elastic across its full service temperature range.
To bond it to butyl, we use a solvent-borne rubber-polymer primer at roughly 5 m²/L. The solvent swells the aged rubber surface slightly while the primer’s rubber soaks into it. Instead of a sharp line between old and new, you get a blended zone where the two are knitted together.
Strengths
- Among the toughest liquid-applied coatings, with high tensile strength, tear resistance and abrasion resistance.
- The right choice where the roof carries foot traffic, service access or walkways.
- Stays elastic for life, which gives it a large reserve for bridging cracks.
- Holds its colour well.
Limitations
- Water sitting on it for long periods softens a water-based film, so dead-flat areas and blocked outlets are its weak point. It needs a minimum fall of about 2°.
- More sensitive to weather during application.
- A mid-grey finish gives up most of the available heat benefit.
System B: High-solids moisture-cure silicone
A single-component, high-solids coating. It’s 50 to 60% silicone polymer by weight (silanol-terminated polydimethylsiloxane), with a crosslinking silane to cure it, titanium dioxide for colour and reflectance, and an aminosilane adhesion promoter. Volume solids typically run 93 to 97%, so the wet film and dry film are close to the same thickness. It cures by reacting with moisture in the air.
The type of crosslinker decides what the film gives off as it cures. Oxime-cure products release methyl ethyl ketoxime. Alkoxy-cure products release methanol or ethanol. Both are current and compliant, and the industry is moving toward alkoxy on health grounds.
Bonding silicone to butyl is a two-stage job. First, a chemical surface activator oxidises and modifies the rubber surface. Then a two-part water-borne epoxy primer goes on as a bridging layer. The epoxy must be overcoated within its stated window (typically 48 hours), or the chemical bond won’t form.
Strengths
- Very hard to beat on ponding water. The cured film repels water and does not re-emulsify when it sits wet.
- Its UV resistance is built into the chemistry rather than added as a formulation package.
- High solids allow single-pass application on shallow falls.
- A white finish removes the largest share of heat load.
- Long-term outdoor exposure studies of up to 40 years show retained adhesion and elastic recovery.
Limitations
- It picks up dirt. Initial reflectance of about 0.88 drops to 0.60 to 0.65 within 3 to 5 years.
- Slippery when wet, with low abrasion resistance.
- Once applied, it commits the roof to silicone chemistry permanently.
Comparative performance

Neither system wins outright. Polyurethane comes out ahead on toughness, movement tolerance and holding its appearance. Silicone comes out ahead on water, UV, heat and ease of renewal. The right choice depends on what is most likely to go wrong on the roof in front of you.
Service life and end of service
Polyurethane
A correctly applied aliphatic polyurethane system gives 10 to 15 years, with a topcoat refresh every 5 to 7 years under New Zealand UV.
To renew it, clean the surface, abrade lightly and apply a fresh topcoat. After about two or three cycles, the built-up film needs stripping back to the sheet. In return, polyurethane keeps your options open. A silicone conversion is still available later.
Silicone
A silicone system at 0.5 to 0.8 mm dry film gives 15 to 25 years. Manufacturer warranty tiers of 10, 15 and 20 years are set against dry film thickness.
To renew it, wash the roof, spot-prime any wear-through and apply a fresh coat. No activator or primer is needed over sound existing film. Renewal is commonly 50 to 70% of the original cost. Each cycle gives another 10 to 15 years, and the cycle can be repeated indefinitely.
CAUTION: Once a roof is coated in silicone, every later coat must be silicone too, unless the film is mechanically removed back to the substrate or a cover board and new membrane are installed. Both options are costly. Almost nothing else bonds reliably to cured silicone. Acrylic and polyurethane applied over cured silicone have a documented pattern of peeling off in sheets, usually at seams and penetrations, usually after thermal cycling, and often years later.
Note: Renewal isn’t automatic even within the same chemistry. A heavily weathered silicone film may need a tie-coat or mechanical abrasion. Run an adhesion test patch, leave it to cure for at least 24 hours, and check it before committing to a full recoat.
Selection guidance
Based on the points above, this is how we’d usually decide:
- Foot traffic, service access or walkways: polyurethane. It’s tougher and more abrasion-resistant, and silicone is slippery when wet.
- Ponding water, dead-flat areas or falls below about 2°: silicone. Long periods of standing water soften a water-based polyurethane film.
- Keeping future options open: polyurethane. A silicone conversion is still possible later, while silicone commits the roof to silicone for good.
- Lowest heat load: white silicone. A white finish removes the largest share of heat load, and a mid-grey polyurethane gives up most of that benefit.
- Appearance over time: polyurethane. It holds its colour well, while silicone picks up dirt and loses reflectance within 3 to 5 years.
- Longest life between recoats and simpler renewal: silicone. It gives 15 to 25 years, and renewal needs no activator or primer over sound film.
Where conditions conflict, water and ultraviolet should outrank cost and appearance. A coating that fails early under standing water or ultraviolet is the most expensive outcome available.
Watch out for
Liquid coatings have had some bad press in New Zealand lately, with homeowners left with peeling, blistering coatings and leaks within months of the job. From what’s been reported, the problem usually isn’t the idea of coating a roof. It’s skipped repairs, poor preparation and priming, and work signed off before anyone checked it.
Before you go ahead with a coating on a butyl roof, ask:
- Which product is it, and is it approved by the manufacturer for use over butyl? Some coatings sold for roof restoration aren’t suited to butyl at all.
- Will they do a moisture survey and a field adhesion test before the main job?
- Which activator or primer will they use, and will it be overcoated within its stated window?
- Will the repairs to seams, flashings, fixings and any rotten deck be done before coating, not coated over?
- Who checks the finished job, and is the dry film thickness recorded? Don’t pay the final invoice until any promised quality check has been done.
- What does the warranty actually cover, who backs it, and how long do you have to make a claim?
A cheap coating that peels off in a couple of years usually ends up costing more than doing it properly the first time, and it can leave the roof in worse shape than before.
Specification and quality checklist
Twelve items. Every one is here because leaving it out has caused a documented failure.
- Moisture survey: an infrared survey to ASTM C1153 or a capacitance survey, with invasive moisture readings of the substrate at any suspect areas, then patched. On a built-up warm roof, core samples may also be needed.
- Cut out the bad areas: wet insulation and unsound sheet cut out and replaced in like material, with at least 48 hours’ drying before any liquid-applied product.
- Adhesion test: on the actual membrane after the planned preparation, cured for the full stated period, to ASTM D3359 or D4541.
- Falls and drainage: written confirmation that falls are positive and all outlets, sumps and overflows are clear and working.
- Metalwork first: all fixings, flashings and sheet metal repaired or replaced before coating, and chloride (salt) deposits removed in corrosion zones C and D.
- Preparation spelled out: wash method, pressure, cleaning agent, dwell time, rinse to clear water, and drying period.
- Primer or activator named: with its coverage rate, and its overcoating window stated as a hard constraint.
- Details reinforced: every moving joint, upstand, penetration, drain and terminating edge reinforced with a three-course fabric or tape detail before the field coats.
- Coverage per coat: specified in litres or kilograms per square metre, tied directly to the warranty term being sought.
- Film thickness checked: wet film checked continuously with a gauge during application; dry film confirmed with small cut tests at a stated frequency, patched afterwards, and recorded before invoicing.
- Conditions logged daily: substrate temperature, air temperature, relative humidity, and the forecast across the cure period.
- Proper handover: the achieved dry film record, warranty registration, a written maintenance schedule, and a clear statement of the chemistry limits on future recoats.
Referenced standards
- NZBC B2: Durability
- NZBC E2: External Moisture
- NZS 3604: wind and corrosion zones
- AS 4654.1 / 4654.2: above-ground membranes
- ASTM D6694: silicone roof coatings
- ASTM D4798 / G154: accelerated weathering
- ASTM C1153: infrared survey for wet roof insulation
- ASTM D3359 / D4541 / D903: adhesion
- ASTM D2370: tensile strength and elongation
- ASTM D624: tear resistance
- ASTM E96: water vapour transmission
- ASTM C1549: solar reflectance
- ASTM E1980: Solar Reflectance Index (SRI)
- NRCA: Guidelines for Roof Coatings
Note: No ASTM specification directly covers water-based aliphatic polyurethane roof coatings. For System A, the manufacturer’s appraisal or technical datasheet governs.